Steel, which confidently holds a blow in summer, can crack like glass in winter. This phenomenon is called cold breaching, and it has cost engineers a lot of high-profile accidents: from cracks in the hulls of wartime ships to the destruction of pipelines and reservoirs in the northern regions. Below we will talk about what happens to the metal when the temperature drops, how it is measured and which errors most often distort the test result.
What is the transition from a viscous to a brittle state?
Most structural steels with a volume-centered cubic lattice break down visibly at room temperature: before cracking, the metal is noticeably deformed and absorbs a lot of energy. As the dislocation cools, the mobility of the dislocations decreases, and in a certain temperature range, the nature of the fracture changes. The crack begins to spread almost without plastic deformation, the fracture becomes shiny and crystalline, and the absorbed energy drops significantly.
This interval is called the temperature of the visco-brittle transition. For one steel grade, it may differ depending on the melting, the thickness of the rolled product, the heat treatment mode, and even the direction of sample cutting. Therefore, the passport value of the brand is not enough: the transition temperature must be confirmed by testing a specific batch.
Austenitic stainless steels, aluminum and copper with a face-centered lattice do not have such a sharp transition. Therefore, they are used in cryogenic technology, where operating temperatures reach the temperature of liquid nitrogen and below.
How is the tendency to brittle fracture measured?
The main evaluation method is called the impact bending test. A standard incised sample is made of metal, cooled to a preset temperature, and destroyed with a single stroke of a pendulum hammer. By the difference in the heights of the pendulum before and after impact, the fracture work is determined, and by referring it to the cross-sectional area under the incision, the impact strength, for example, KCV or KCU, in J /cm2, is obtained.
To build a complete picture, the tests are carried out at several temperatures: for example, +20, 0, -20, -40, -60 ° C. Based on the results, a serial curve is constructed, which clearly shows the "upper shelf" of viscous fracture, the "lower shelf" of brittle and the transition region between them. Additionally, the proportion of the viscous component in the fracture is estimated: it is determined visually or from a photograph of the fracture.
Product standards usually require that the impact strength be confirmed at a single reference temperature. For metal structures that are operated in cold climates, it is often -40 or -60 °C, and for Arctic-type equipment and liquefied gases, the requirements are even stricter.
Impact strength is not included in the strength calculation formulas. This is a comparative indicator that